Note: The Table chart below gives typical mechanical characteristics for selected carbon steel properties. For all critical applications, verify to the applicable industry or requisite material / steel standard.

AISI Reference
Manufactured
Strength
Elongation
(%)
Hardness,
Bhn
Tensile
Yield
psi (lb/in.2)
1015
Hot Rolled
Normalized (1700 F)
Annealed (1600 F)
61,000
61,500
56,000
45,500
47,000
41,250
39.0
37.0
37.0
126
121
111
1020
Hot Rolled
Normalized (1600 F)
Annealed (1600 F)
65,000
64,000
57,250
48,000
50,250
42,750

36.0
35.8
36.5

143
131
111
1022
Hot Rolled
Normalized (1700 F)
Annealed (1600 F)
73,000
70,000
65,250
52,000
52,000
46,000
35.0
34.0
35.0
149
143
137
1030
Hot Rolled
Normalized (1700 F)
Annealed (1550 F)
80,000
75,000
67,250

50,000
50,000
49,500

32.0
32.0
31.2
179
149
126
1040
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
90,000
85,500
75,250
60,000
54,250
51,250
25.0
28.0
30.2
201
170
149
1050
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
105,000
108,500
92,250
60,000
62,000
53,000
20.0
20.0
23.7
229
217
187
1060
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
118,000
112,500
90,750
70,000
61,000
54,000
17.0
18.0
22.5
241
229
179
1080
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
140,000
146,500
89,250
85,000
76,000
54,500
12.0
11.0
24.7
293
293
174
1095
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
140,000
147,000
95,250
83,000
72,500
55,000
9.0
9.5
13.0
293
293
192
1117
Hot Rolled
Normalized (1650 F)
Annealed (1575 F)
70,600
67,750
62,250
44,300
44,000
40,500
33.0
33.5
32.8
143
137
121
1118
Hot Rolled
Normalized (1700 F)
Annealed (1450 F)
75,600
69,250
65,250
45,900
46,250
41,250
32.0
33.5
34.5
149
143
131
1137
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
91,000
97,000
84,750
55,000
57,500
50,000
28.0
22.5
26.8
192
197
174
1141
Hot Rolled
Normalized (1650 F)
Annealed (1500 F)
98,000
102,500
86,800
52,000
58,750
51,200
22.0
22.7
25.5
192
201
163
1144
Hot Rolled
Normalized (1650 F)
Annealed (1450 F)
102,000
96,750
84,750
61,000
58,000
50,250
21.0
21.0
24.8
212
197
167
1340
Normalized (1600 F)
Annealed (1475 F)
121,250
102,000
81,000
63,250
22.0
25.5
248
207

Related: